347 VS 347H VS 347HFG

                   

ASTM A213 347/347H / 347HFG Stainless Steel Tubes Chemical Composition

Grade347347H347HFG
UNS DesignationS34700S34709S34710
Carbon (C) Max.0.080.04–0.100.06–0.10
Manganese (Mn) Max.2.002.002.00
Phosphorous (P) Max.0.040.040.04
Sulphur (S) Max.0.030.030.03
Silicon (Si) Max.0.750.750.75
Chromium (Cr)17.0–20.017.0–20.017.0–20.0
Nickel (Ni)9.0–13.09.0–13.09.0–13.0
Molybdenum (Mo)
Nitrogen (N)
Iron (Fe)Bal.Bal.Bal.
Other ElementsCb+Ta=10xC-1.0Cb+Ta=8xC-1.0Nb+Ta=8xC-1.0

347 347H 347HFG Stainless Steel Mechanical Properties

Tensile StrengthTensile StrengthYield StrengthYield Strength
AlloyUNSSpecMPaksiMPaksiElongation in 2 inches (min.) %Harndess
HBW
347S34700ASTM
A213
515752053035192
347HS34709ASME SA 213515752053035192
347HFGS34710550802053035192

347 347H 347HFG Stainless Steel Physical Properties

AlloyUNS
Design
Density kgs/dm³Modulus of Elasticity
(x106 psi)
Mean Coefficient of Thermal Expansion (IN./IN./°F x 10-6)Thermal Conductivity (BTU-in/ft2-h-°F)
347S347007.9829.09.2
347HS347097.9829.09.2
347HFGS3471029.09.2

347 347H 347HFG Stainless Steel Grain Size

AlloyUNSSpecGrain Size Req. ASTM E112
347S34700ASTM
A213
347HS34709ASME SA 2137 or coarser
347HFGS34710ASME SA2137 – 10
304H

347 347H General Properties
347 347H Chemical Composition
347 347H Resistance to Corrosion
347 347H Physical Properties
347 347H Mechanical Properties
347 347H Elevated Temperature Oxidation Resistance
347 347H Heat Treatment
347 347H Fabrication

Related Articles