Material |
Yield strength
(MPa) |
Ultimate strength
(MPa) |
Density
(g/cm³) |
ASTM A36 steel |
250 |
400 |
7.8 |
Steel, API 5L X65 (Fikret Mert Veral) |
448 |
531 |
7.8 |
Steel, high strength alloy ASTM A514 |
690 |
760 |
7.8 |
Steel, prestressing strands |
1650 |
1860 |
7.8 |
Piano wire |
2200–2482[5] |
|
7.8 |
High density polyethylene (HDPE) |
26-33 |
37 |
0.95 |
Polypropylene |
12-43 |
19.7-80 |
0.91 |
Stainless steel AISI 302 - Cold-rolled |
520 |
860 |
|
Cast iron 4.5% C, ASTM A-48 |
276 (??) |
200 |
|
Titanium alloy (6% Al, 4% V) |
830 |
900 |
4.51 |
Aluminium alloy 2014-T6 |
400 |
455 |
2.7 |
Copper 99.9% Cu |
70 |
220 |
8.92 |
Cupronickel 10% Ni, 1.6% Fe, 1% Mn, balance Cu |
130 |
350 |
8.94 |
Brass |
approx. 200+ |
550 |
5.3 |
Tungsten |
|
1510 |
19.25 |
Glass |
|
50 (in compression) |
2.53 |
E-Glass |
N/A |
3450 |
2.57 |
S-Glass |
N/A |
4710 |
2.48 |
Basalt fiber |
N/A |
4840 |
2.7 |
Marble |
N/A |
15 |
|
Concrete |
N/A |
~50 compression |
23.6kN/m2; |
Carbon fiber |
N/A |
5650 |
1.75 |
Spider silk |
1150 (??) |
1200 |
|
Silkworm silk |
500 |
|
|
Aramid (Kevlar or Twaron) |
3620 |
|
1.44 |
UHMWPE |
23 |
46 |
0.97 |
UHMWPE fibers[6][7] |
|
2300-3500 |
0.97 |
Vectran |
|
2850-3340 |
|
Pine wood (parallel to grain) |
|
40 |
|
Bone (limb) |
104-121 |
130 |
|
Nylon, type 6/6 |
45 |
75 |
|
Rubber |
- |
15 |
|
Boron |
N/A |
3100 |
2.46 |
Silicon, monocrystalline (m-Si) |
N/A |
7000 |
2.33 |
Silicon carbide (SiC) |
N/A |
3440 |
|
Sapphire (Al2O3) |
N/A |
1900 |
3.9-4.1 |
Carbon nanotube (see note above) |
N/A |
62000 |
1.34 |